Original
Open Access
Mathematical model for galvanic corrosion of steel–copper couple in petroleum waste water in presence of friendly corrosion inhibitor
Visits
7125
Anees A. Khadoma,
Corresponding author
aneesdr@gmail.com

Corresponding author.
, Baker M. Abodb
a Chemical Engineering Department, College of Engineering, University of Diyala, Baquba City, Diyala, Iraq
b Technical Engineering College, Middle Technical University, Baghdad, Iraq
This item has received

Under a Creative Commons license
Article information
Abstract
Full Text
Bibliography
Download PDF
Statistics
Figures (9)
Show moreShow less
Tables (2)
Table 1. Solubility of oxygen in 1% MgCl2.
Tables
Table 2. Galvanic corrosion of Cu/Fe couple versus temperature under the following conditions: [Fe2+]=[Zn2+]=10−6M, fFe=0.5, fZn=0.5, alpha of H2=0.5, alpha of Cu=Fe=0.5.
Tables
Show moreShow less
Abstract

Galvanic corrosion of steel–copper couple in saline petroleum wastewater in the absence and presence of curcuma extract as corrosion inhibitor was studied as a function of temperature, velocity, and inhibitor concentration. The electrochemical polarization technique was used to evaluate the corrosion parameters. Corrosion currents densities increase with temperature and velocity, while it decreases with inhibitor concentrations. In this investigation, a theoretical model equation was used to analyze the shape of polarization curves. Microsoft Excel program was used to find the galvanic current and galvanic potential. Theoretical results agreed with experimental one.

Keywords:
Galvanic corrosion
Electrochemical measurements
Numerical solution
Microsoft Excel
Full Text
1Introduction

Corrosion is a chemical or electrochemical reaction between a metal and its environment that produce degradation of material. There are several kinds of corrosion such as uniform corrosion, galvanic corrosion, crevice corrosion, pitting, intergranular corrosion, etc. Galvanic corrosion happens when a metal or alloy is electrically coupled to another metal in same the environment. There are many methods of corrosion control such as material selection, coatings, inhibitors, and cathodic protection. Corrosion inhibitor is organic or inorganic component that can be added in small amounts to reduce corrosion problems (Khadom, Yaro, AlTaie, & Kadum, 2009a; Khadom, Musa, Kadhum, Mohamad, & Takriff, 2010; Musa, Khadom, Kadhum, Takriff, & Mohamad, 2012). Recently the using of friendly and the natural materials where the aim of researchers that concentrated on studying the kinetics parameters, such as, activation parameters and adsorption behavior of the corrosion inhibition process (Yaro, Khadom, & Ibraheem, 2011a; Yaro, Khadom, & Wael, 2013; Yaro, Khadom, & Wael, 2014). Application of mathematical modeling was rarely used. Mathematical modeling is a powerful tool for increasing the availability of electrochemical data for a number of materials and environmental systems for industrial applications that enable chemical and materials engineers to predict corrosion potentials and corrosion rates using equations derived from electrochemical principles (Khadom & Yaro, 2011; Khadom, Yaro, Altaie, & Kadhum, 2009b). The present work was a step in the direction of application a mathematical model for galvanic corrosion – saline water – inhibitor system at different operating conditions.

2Mathematical model

For activation control and to determine the potential of a system, in which the reduced and oxidized species are not at unit activity, the familiar Nernest equation can be employed (Cifuentes, 1987; Fontana, 1987):

or written as:
where E is the equilibrium half-cell potential, Eo the standard equilibrium half-cell potential, R is the gas constant (8.314J/Kmol), T is the absolute temperature (K), n is the number of electrons transferred, F the Faraday constant (96,487coulomb/equiv.), ared and aoxid are activities or (concentrations) of oxidized and reduced species. Hydrogen ion activity is commonly expressed, for convenience, in terms of pH. This is defined as (Uhlig & Revie, 1985):
Hence, for the half-cell reaction

Tafel slopes (Tafel constants) are determined from the following equations (Fontana, 1987):

for anode and cathode reaction, respectively, where α is the symmetry coefficient, which describes the shape of the rate controlling energy barrier. The relationship between reaction rate and overvoltage for activation polarization is:
where ηA is overvoltage, β as before, and i is the rate of oxidation or reduction in terms of current density. This equation is called the Tafel equation. The reaction rate is given by the reaction current or current density, so the high field approximation gives (Uhlig & Revie, 1985):
and
The effect of temperature is to change the value of the exchange current density io as follows (Uhlig & Revie, 1985):

Corrosion current for anodic reaction rate can be obtained as (Uhlig & Revie, 1985):

and the cathodic one is:

For the case of diffusion control, the reaction current is given by Fick's law (Liberati, Nogueira, Leonel, & Chateauneuf, 2014):

or its equivalent

The limiting current, i.e. the maximum current under diffusion control is obtained when Cs=0, so

or
where the mass transfer coefficient is defined as

The corrosion current is then

zc is used in Eqs. (15)–(20) because in corrosion processes the cathodic reaction is the one likely to be controlled by diffusion. Cb solubility of oxygen in water. The bulk concentration of oxygen changes with pressure, for barometric pressures other than 101.325kPa (sea level), the bulk concentration of oxygen can be computed from the following equation (Truesdale, Downing, & Lowden, 1955):
where Cb is the bulk concentration of oxygen, C101.325 is a saturation value at 101.325kPa (tested experimentally, Table 1), PT is total pressure (kPa), p is the vapor pressure of water. The mass transfer coefficient (K) in Eq. (19) varies with the flow or relative speed between metal and the environment, the geometry of the system and the physical properties of the liquid. To calculate the variation of K in dynamic environment, dimensionless group are used such as (Yaro, Al-Jendeel, & Khadom, 2011b):

Table 1.

Solubility of oxygen in 1% MgCl2.

Temperature (°C)  Concentration of inhibitor (ppm)  Solubility of oxygen (mg/l) 
30Blank 
90  5.9 
180  5.8 
270  5.8 
360  5.8 
35Blank  5.8 
90  5.6 
180  5.6 
270  5.5 
360  5.5 
40Blank  5.6 
90  4.6 
180  4.6 
270  4.6 
360  4.5 

All are often applied. For the smooth rotating cylinder electrode, the mass transport correlation is given by Eisenberg, Tobias, and Wilke (1954) relationship applies in the case of turbulent regime.

The value of K from Eqs. (22)–(25) can be expressed as:

This correlation is valid within the following range: 1000<Re<100000 and 850<Sc<11490. The effect of temperature and pressure on diffusion coefficient is shown in the following equation:

where the exponent n varies from 1.75 to 2.0, To reference temperature in K, Do diffusion coefficient at the reference temperature and pressure, Po reference pressure. For galvanic corrosion under activation control (Hassan, Abdul Kader, & Abdul-Jabbar, 2011) at (Eg):
And
for one metal
for two metals
or in terms of current densities and areas
Or
if Ia.1Ia.2, Eq. (31) reduce to

Ee.c1=Ee.c2=Ee.c and αc1=αc2=αc

for diffusion control (Hassan et al., 2011):
for one metal
for two metals
where f1 and f2 are the anodic and cathodic electrode area fractions.

Eq. (47) became

For binary galvanic system under activation control (acidic medium) and mass transfer (diffusion) control (neutral medium),

for one metal:

when two metals at (Eg):

3Experimental work3.1Preparation of plant extracts

Fresh Curcuma longa (turmeric) were washed under running water, sliced into small pieces before drying in a hot air oven at 50°C for about 6h. Dry slice was collected and ground into fine powder using a high-speed blender. The dry, Curcuma longa was packed in a plastic bag, sealed, and kept until used. The slice (25g) was blended with distilled water (250ml) in a reflux heater with conical flax (500ml) for 3h at 70°C. The conical flax was supplied with mixer for homogenous solution and uniform temperature distribution. The solution is then cooled, followed by filtration to extract solid particles free inhibitor solution. Each 1cm3 of extract yield a powder 0.0045g of solid material.

3.2Polarization tests

A total of 90 test runs was carried out in the presence and absence of inhibitor at different experimental conditions using potentiodynamic polarization technique. Tests were carried out using a beaker of 500ml. The cell containing working electrode, lugging capillary probe, thermometer, counter graphite electrode. All potential values were measured in reference to a saturated calomel electrode (SCE). The lugging capillary prob was adjusted such that it was at a distance not more than 1mm from the working electrode. The working electrode were 2 samples from carbon steel type (ASTM A 106/A) and copper type (ASTM B-111-443). The working electrode was (2.4cm outside diameter x 1.35cm long) carbon steel (type ASTM A 106/A) and copper (type ASTM B-111-443) cylinder; this cylinder was fixed on brass zone on the shaft. Graphite electrode was used as a counter electrode has a dimension of (9.5cm diameter×8cm. long), two wires were connected to a cylindrical concentric graphite electrode. The chemical compositions (% wt) of working electrodes were for steel alloy 0.25%C, 0.5%Mn, 0.025%P, 0.025%S, 0.1%Si, 0.4%Cr, 0.15%Mo, and the balance is Fe. The copper alloy compositions are 70–73%Cu, 0.007%Pb, 0.0006%Fe, 0.001%Sb, 0.0.009%Sn, and the balance is Zn. Mild steel and copper specimens were cleaned using emery paper of grade number 220, 320, 400, and 600, then washed with running tap water followed by distilled water, then dried with a clean tissue, degreased with benzene, dried, degreased with acetone, dried, and finally left in desiccator over silica gel. The electrode was mounted directly to the working electrode. (SCE) was used as a reference electrode. To ensure that KCl solution was saturated, a small amount of KCl (solid) was kept in the solution of (SCE) as long as the test. The cathodic polarization is carried out beginning from the highest negative potential of −900mV until reaching the corrosion potential. The potential was changed in scan rate of 10–15mV/min, then the current is recorded. The anodic polarization readings start of a potential resulting in a zero current density and is increased in a step of 10–15mV with recording of the current at each step for one minute interval until a potential of about −100mV. The galvanic corrosion rate of steel–copper couple in the absence and presence of inhibitor concentration of 0, 90, 180, 270 and 360ppm, area ratio of cathode to anode 1:1, at different temperature 30, 35, and 40°C was evaluated in aerated 1% (wt) MgCl2 and pH 6.

4Results and discussion4.1Electrochemical polarization studies

The corrosion behavior of Fe and Cu in 1% MgCl2 solution with and without inhibitor was studied using polarization techniques. The inhibitor was tested in different conditions of temperature, velocity and inhibitor concentration. A total of 90 test runs is carried out. Electrochemical parameters for each metal individually were calculated using polarization curves similar to Figures 1 and 2 that obtained for Fe and Cu in 1% MgCl2 solution. While galvanic parameters were calculated by superimposing the anodic branch of the less noble material (mild steel) to the cathodic branch of the most noble material (copper alloy) as shown in Figure 3. Similar figures are obtained at all operating conditions. From polarization curves, the free corrosion current Icorr, corrosion potential Ecorr, limiting current density, iL, and galvanic corrosion, Ig were obtained. A plateau corresponding to a limiting current density (il) is observed in the cathodic region of the polarization curves between −800 and −600mV SCE. Therefore, the cathodic reaction seems to be controlled by diffusion. It was shown that the values of Icorr and Ig increased with temperature and velocity, while it decreased with inhibitor concentration. Maximum inhibitor efficiency was around 90% at 360ppm and 30°C. The average values of inhibitor efficiency were approximately 55, 72, 76, and 83% at inhibitor concentration of 90, 180, 270, and 360ppm respectively. The increasing in corrosion protection with addition of inhibitor may be attributed to increase in metal surface coverage. Increasing inhibitor concentration beyond 380ppm may yield further reduction in galvanic corrosion current, but economical considerations have to be taken into account. Figures 4 and 5 show the variation of galvanic corrosion as a function of different operating conditions.

Fig. 1.

Polarization curves for the corrosion of Fe in 1% wt MgCl2 at temperature 30°C and different rotation speed.

Fig. 2.

Polarization curves for the corrosion of Cu in 1% wt MgCl2 at temperature 30°C and different rotation speed.

Fig. 3.

Polarization curves for the corrosion of Fe–Cu coupling at speed of rotation 50rpm, temperature 40°C and 180ppm inhibitor concentration.

Fig. 4.

Galvanic current as a function of speed of rotation at different temperature in absence of inhibitor.

Fig. 5.

Galvanic current as a function of temperature at different inhibitor concentration.

4.2Theoretical and modeling studies

A mathematical model has been developed based on the ordinary galvanic corrosion model and fluid dynamics analysis model. The calculation is divided into two types. Activation control and mass transfer control. Simplifications leading to analytic solutions of the model equations are so complex, so numerical solutions must be attempted. As an example, a numerical method implemented on a microcomputer. The sweeping method and algorithm are as follows:

  • 1.

    Estimate equilibrium potentials for metals and for hydrogen from Eq. (1) at T of 30, 35 and 40°C. For pH values use Eq. (3) to calculate hydrogen ion concentrations.

  • 2.

    Tafel slopes for anodic and cathodic reactions are established from Eqs. (4) and (5) at α=0.5 and T of 30, 35 and 40°C.

  • 3.

    The exchange current density is calculated from Eq. (10) for three values of temperatures (30, 35 and 40°C).

  • 4.

    Bulk concentration of oxygen in water is calculated from Eq. (21) at different temperatures 30, 35 and 40°C, by using, Table 1.

  • 5.

    The value of oxygen diffusivity is estimated from Eq. (27) at different temperatures 30, 35 and 40°C. The mass transfer coefficient K is calculated by using Eq. (26).

  • 6.

    The limiting current is estimated from Eq. (20) at different temperatures 30, 35 and 40°C.

  • 7.

    It is necessary to realize that the galvanic corrosion potentials (Eg) of the reactions involved are chosen between the more negative (or less positive) equilibrium potential of the metals and the equilibrium potential of hydrogen evolution.

  • 8.

    The values of Eeq, β, io, Eg (=Ea=Ec) are substituted in Eqs. (11) and (13) to determine anodic and cathodic currents.

  • 9.

    For activation control:

  • 10.

    The summations of the anodic and cathodic currents are compared to determine the absolute value of their difference.

  • 11.

    A new value of Eg is assumed as in step 8 and the program is executed again, showing the difference between the summation of the anodic and cathodic currents to decrease

  • 12.

    Step 11 is repeated until a minimum difference current is found. The minimum will be detected when the sweeping procedure goes beyond the true galvanic potential value as the difference starts increasing. The precision will be greater the smaller the potential step while the processing time will increase accordingly.

  • 13.

    For mass transfer control:

  • 14.

    The difference between the summation of the anodic currents and limiting currents, Eq. (42), are calculated and compared to determine the absolute value of their difference.

  • 15.

    A new value of Eg is assumed as in step 8 and the program is executed again, showing the difference between the summation of the anodic and limiting currents to decrease

  • 16.

    Step 11 is repeated until a minimum difference is found. The minimum will be detected when the sweeping procedure goes beyond the true galvanic potential value as the difference starts increasing. The precision will be greater the smaller the potential step while the processing time will increase accordingly.

  • 17.

    For cathode reaction under activation control complicit with mass transfer:

  • 18.

    The difference between the summation of the anodic and cathodic currents and limiting currents Eq. (49), are calculated and compared to determine the absolute value of their difference.

  • 19.

    A new value of Eg is assumed as in step 8 and the program is executed again, showing the difference between the summation of the anodic and cathodic currents and limiting currents to decrease

  • 20.

    Step 11 is repeated until a minimum difference is found. The minimum will be detected when the sweeping procedure goes beyond the true galvanic potential value as the difference starts increasing. The precision will be greater the smaller the potential step while the processing time will increase accordingly.

A program written in Microsoft Excel 2010 for free corrosion rate of single metal and binary galvanic system under activation control (acidic medium) and mass transfer (diffusion) control (neutral medium) and also to calculate the galvanic corrosion rate when the system is under both activation and mass transfer control. Table 2 that shows the effect of temperature on the corrosion current and corrosion potential of copper and iron, limiting current was calculated from Eq. (44), corrosion current of metals were calculated from Eq. (53). Figures 6 and 7 show a comparison of the galvanic current density obtain from polarization curve and theoretical calculation. Figures 8 and 9 show a comparison of the galvanic current density obtain from polarization curve, weight loss and theoretical calculation.

Table 2.

Galvanic corrosion of Cu/Fe couple versus temperature under the following conditions: [Fe2+]=[Zn2+]=10−6M, fFe=0.5, fZn=0.5, alpha of H2=0.5, alpha of Cu=Fe=0.5.

T (°C)  rpm  Eg (mV)  ICu (μA/cm2IFe (μA/cm2IH2/Cu   (μA/cm2)  IH2/Fe   (μA/cm2)  ILimiting (μA/cm2
30  0−0.79537  1.094E−11  57.332  3.23710  0.9141  53.1813 
35  −0.83150  2.555E−12  59.644  1.91495  1.1058  56.6239 
40  −0.83578  8.056E−12  66.779  1.71268  0.8241  64.2429 
30  50−0.82944  2.062E−12  65.240  4.25687  1.7317  59.2514 
35  −0.83656  2.957E−12  64.116  3.31561  1.1878  59.6125 
40  −0.83968  9.196E−12  62.836  1.45716  0.8992  60.4799 
30  200−0.79930  7.466E−12  158.870  1.59136  0.8795  156.399 
35  −0.80699  1.663E−11  159.46  1.48002  0.6337  157.352 
40  −0.81276  3.079E−11  160.84  0.72399  0.4773  159.642 
Fig. 6.

Comparison of the galvanic current density obtains from polarization curve and theoretical calculation at temperature 30°C different rpm.

Fig. 7.

Comparison of the galvanic current density obtains from polarization curve and theoretical calculation at temperature 35°C different rpm.

Fig. 8.

Comparison of the galvanic current density obtains from polarization curve, weight loss and theoretical calculation at different temperature.

Fig. 9.

Comparison of the galvanic current density obtains from polarization curve and theoretical calculation at different temperature and rpm.

5Conclusion

Galvanic current and the corrosion current densities increase with increasing temperature and velocity, and decrease with increasing inhibitor concentrations. The addition of inhibitor reduced the galvanic corrosion current. A mathematical model equation was very effective tool to analyze the shape of polarization curves. Theoretical results agreed with experimental one.

Conflict of interest

The authors have no conflicts of interest to declare.

Acknowledgment

The authors would like thanks Prof. Dr. Apreal S. Yaro (Baghdad University – Chemical Engineering Department) for his continuous encouragement and assistance.

References
[Cifuentes, 1987]
L. Cifuentes.
Electrochemical kinetics helps quantify corrosion phenomena.
Anti-Corrosion, Methods and Materials, 34 (1987), pp. 4-9
[Eisenberg et al., 1954]
M. Eisenberg, C.W. Tobias, C.R. Wilke.
Ionic mass transfer and concentration polarization at rotating electrodes.
Journal of the Electrochemical Society, 101 (1954), pp. 306-320
[Fontana, 1987]
M. Fontana.
Corrosion engineering.
McGraw-Hill, (1987),
[Hassan et al., 2011]
B. Hassan, H. Abdul Kader, M. Abdul-Jabbar.
Experimental study on carbon steel corrosion and its inhibition using sodium benzoate under different operating conditions.
Journal of Chemical and Petroleum Engineering, 12 (2011), pp. 11-24
[Khadom and Yaro, 2011]
A.A. Khadom, A.S. Yaro.
Modeling of corrosion inhibition of copper–nickel alloy in hydrochloric acid by benzotriazole.
Russian Journal of Physical Chemistry A, 85 (2011), pp. 2005-2012
[Khadom et al., 2010]
A.A. Khadom, A.Y. Musa, A.A.H. Kadhum, A.B. Mohamad, M.S. Takriff.
Adsorption kinetics of 4-amino-5-phenyl-4H-1, 2, 4-triazole-3-thiol on mild steel surface.
Portugaliae Electrochimica Acta, 28 (2010), pp. 221-230
[Khadom et al., 2009a]
A.A. Khadom, A.S. Yaro, A.S. AlTaie, A.A.H. Kadum.
Electrochemical, activations and adsorption studies for the corrosion inhibition of low carbon steel in acidic media.
Portugaliae Electrochimica Acta, 27 (2009), pp. 699-712
[Khadom et al., 2009b]
A.A. Khadom, A.S. Yaro, A.S. Altaie, A.A.H. Kadhum.
Mathematical modeling of corrosion inhibition behavior of low carbon steel in HCl acid.
Journal of Applied Sciences, 9 (2009), pp. 2457-2462
[Musa et al., 2012]
A.Y. Musa, A.A. Khadom, A.A.H. Kadhum, M.S. Takriff, A.B. Mohamad.
The role of 4-amino-5-phenyl-4H-1, 2, 4-triazole-3-thiol in the inhibition of nickel–aluminum bronze alloy corrosion: Electrochemical and DFT studies.
Research on Chemical Intermediates, 38 (2012), pp. 91-103
[Liberati et al., 2014]
E.A. Liberati, C.G. Nogueira, E.D. Leonel, A. Chateauneuf.
Nonlinear formulation based on FEM, Mazars damage criterion and Fick's law applied to failure assessment of reinforced concrete structures subjected to chloride ingress and reinforcements corrosion.
Engineering Failure Analysis, 46 (2014), pp. 247-268
[Truesdale et al., 1955]
G.A. Truesdale, A.L. Downing, G.F. Lowden.
The solubility of oxygen in pure water and sea-water.
Journal of Applied Chemistry, 5 (1955), pp. 53-62
[Uhlig and Revie, 1985]
H. Uhlig, W. Revie.
Corrosion and corrosion control.
John Wiley and Sons, (1985),
[Yaro et al., 2011a]
A.S. Yaro, A.A. Khadom, H.F. Ibraheem.
Peach juice as an anti-corrosion inhibitor of mild steel.
Anti-Corrosion Methods and Materials, 58 (2011), pp. 116-124
[Yaro et al., 2011b]
A. Yaro, H. Al-Jendeel, A. Khadom.
Cathodic protection system of copper–zinc–saline water in presence of bacteria.
Desalination, 270 (2011), pp. 193-198
[Yaro et al., 2013]
A.S. Yaro, A.A. Khadom, R.K. Wael.
Apricot juice as green corrosion inhibitor of mild steel in phosphoric acid.
Alexandria Engineering Journal, 52 (2013), pp. 129-135
[Yaro et al., 2014]
A.S. Yaro, A.A. Khadom, R.K. Wael.
Garlic powder as a safe environment green corrosion inhibitor for mild steel in acidic media; adsorption and quantum chemical studies.
Journal of the Chinese Chemical Society, 61 (2014), pp. 615-623

Peer Review under the responsibility of Universidad Nacional Autónoma de México.

Copyright © 2017. Universidad Nacional Autónoma de México, Centro de Ciencias Aplicadas y Desarrollo Tecnológico